Resin printers fail in a small number of ways, and each leaves a clue: a bare build plate, a sheet of cured resin on the film, supports with nothing on top, a crater in a wall. This guide shows how to read those clues and fix the cause. If you are setting up for the first time, start with resin printing for beginners.

Wear gloves for every step below. Failed prints mean more liquid resin to handle than usual; see resin printing safety.

First: read the failure

Before you change a setting, look at what is on the plate, what is in the vat, and the layer where things went wrong.

Reading a failed resin print: plate empty with a sheet on the film means levelling, bottom exposure or cold; supports without model means weak supports or low exposure; split layers mean peel force or pauses; a hole in a wall is a cupping blowout; swollen details mean over-exposure; sticky or white after curing comes from washing and curing
Where the print failed tells you what went wrong. Image: PrintStock

Then work through the likely causes in order, cheapest first:

Troubleshooting order for resin printing: temperature, film and vat, plate, exposure, file, hardware
Cheapest and most likely causes first. Image: PrintStock

After any failed print, clear the vat before you print again. Fish out cured fragments with a plastic scraper, or strain the resin through a paint filter. Some printers can expose a thin layer over the whole screen to lift debris as one sheet. A fragment left in the vat can pierce the film or press on the screen on the next print.

The plate comes up empty, with a sheet stuck to the film

The first layers bonded to the film instead of the build plate. This is the most common resin failure.

Causes, from most to least likely:

  • Cold resin. Below about 20 °C, resin cures more slowly and the first layers bond weakly. Warm the room or the printer before you change any setting.
  • Levelling. If the plate sits even slightly too far from the film, the first layers cure on the film. Re-level following your printer's routine.
  • A dirty or smooth plate. Cured resin left on the plate, or a plate polished smooth, holds less well. Clean it with alcohol before every print.
  • Bottom exposure too short or too few bottom layers. Anycubic's own guidance is to add about 10 seconds of bottom exposure and 5 bottom layers, then test again.
  • Lift too short or too fast. If the plate does not rise far enough or rises too quickly, the part can stay on the film. Use the resin maker's lift settings for your printer.

Remove the cured sheet with a plastic scraper or by gently flexing the film from underneath. Never use metal tools on the film.

The model is missing but the supports printed

The supports held, but the model tore off them. The model was too heavy for its supports, or each layer pulled too hard on them.

  • Add supports or make the tips thicker. Look again at the islands and overhangs the slicer reports.
  • Tilt the model. At 30 to 45 degrees each layer is smaller, so the peel force on the supports drops.
  • Check exposure. Under-exposed supports are soft and snap. Run a calibration print such as the Cones of Calibration, which shows support strength directly.
  • Check temperature again. Cold resin is thicker and pulls harder at every lift.

Layers split or the part separates partway up

Layers peeled apart because the forces on them were larger than the bond between them. Formlabs lists the main causes as sudden jumps in layer area (a small layer above a large one), parts that are free-hanging or badly supported, and long pauses during the print.

  • Reorient the part so its cross-section changes gradually, and tilt it to avoid large flat layers.
  • Add supports to anything that starts as a floating island.
  • Avoid pausing prints for long periods.
  • Check the film. A cloudy, loose or damaged film releases layers poorly; see the FEP film guide.

Holes and craters in walls

A hole that grows outward through a wall is a cupping blowout. Formlabs explains it this way: a hollow or cup-shaped section traps a pocket, and as the plate pulls away, the pocket expands and pulls on the wall until it ruptures.

  • Add drain holes near the lowest points of any hollow section, and at least two per cavity.
  • Turn cup shapes so they do not open towards the screen.
  • Thicken thin walls on hollow parts.

Details swollen, holes too small, supports hard to remove

These are signs of over-exposure. Extra light cures resin beyond the edges of each pixel, so details fatten, small holes and gaps fill in, and supports fuse to the surface.

  • Lower normal exposure in small steps and print a calibration model.
  • Recalibrate whenever you change resin, layer height or colour; clear and dark resins behave differently from grey.
  • Check that bottom exposure is not applied to too many layers; it causes a flared base, the resin version of elephant's foot.

The opposite, missing small details and fragile supports, is under-exposure. Raise normal exposure in small steps.

Lines and bands across the print

Regular horizontal lines usually come from something that changed during the print.

  • Temperature drift. If the room cools during a long print, the resin thickens and cures differently, and a band appears where it changed. Keep the temperature steady rather than preheating the resin once.
  • Z axis. A dirty, dry or damaged lead screw or rail can cause repeating bands. Clean and lubricate it as your printer's manual says.
  • Plate or vat not fully tightened. A loose part moves slightly at every lift.
  • Pauses. Opening the lid or pausing a print often leaves a visible line.

Faint, even steps on curved surfaces are normal layer lines; thinner layers and tilting the part make them smaller.

Sticky, white or cloudy parts after curing

These problems come from post-processing, not the printer.

  • Sticky surface. Uncured resin is still on the part: the wash was too short, or the alcohol is saturated with resin. Rewash in clean alcohol, dry, and cure again. Under-curing, or curing in a cold room, can also leave tack.
  • White bloom or chalky film. The part was cured while alcohol or water was still on it. Dry parts until they look dull, blowing air into recesses, before curing. A bloom that is already cured can often be removed with light wet sanding.
  • Cloudy clear resin. Clear resin needs careful exposure and a short cure; Phrozen notes that over-curing makes it cloudy and under-curing leaves it soft and sticky.

The beginner guide covers the full wash, dry and cure routine.

Cracks after curing

Cracks that appear hours or days later usually come from stress inside the part.

  • Over-curing. Long cures make parts brittle. Follow the resin maker's cure time.
  • Thick solid sections. Big solid parts shrink unevenly as they cure. Hollow them, with drain holes.
  • Trapped liquid. Alcohol or uncured resin trapped inside a hollow part can crack it from inside. Drain and dry hollow parts fully.
  • Water-washable resin. Phrozen says water-washable resin tends to be more brittle and can crack, especially in humid conditions. Dry these parts thoroughly and store them dry. See 3D printer resin types.

Hardware problems: screen and light

If every setting is right and failures follow a pattern, check the hardware.

  • Dead areas on the screen. Most printers have a screen test that shows the whole display. Missing lines or patches mean the screen is failing; mono LCD screens are a consumable on resin printers.
  • Uneven light. If parts in one area of the plate fail while others print, the light source may be uneven or the screen protector dirty.
  • Resin under the film. If resin leaked through a damaged film, stop and clean the screen before printing again; see the FEP film guide.

Problems owners report with specific printers

Some problems belong to a particular model rather than to settings. Here are the printers in our catalog where owner reports describe resin, vat or film problems:

Owners report this on 19 of the 370 printers we track

  • Anycubic Photon Mono 4: Early LCD failure from resin leaks; Z axis does not stop at home
  • Anycubic Photon Mono 4 Ultra: False residue and resin warnings; No vat heater
  • Anycubic Photon Mono M7 Max: Auto-fill empties the bottle
  • Anycubic Photon Mono M7 Pro: Auto-fill pump tube cracks and leaks resin; Resin leaks into the chassis; Vat heater only works before the print starts; Noisy fans and heavy, unbalanced vat
  • Anycubic Photon P1: Resin leaks under the vat; Flat plate pools resin; Dual mode limits
  • Anycubic Photon P1 Max: Thick early layers waste resin; Flat, heavy build plate; No auto-refill and no dual vat
  • Elegoo Jupiter 2: Features missing or immature at launch; Pump hose leaks and clogs; Resin pump and bottle placement; Cumbersome vat removal
  • Elegoo Mars 3: No carbon filter or lid gasket
  • Elegoo Mars 5 Ultra: Self-test messages block printing; Cold resin causes failures; Resin leaks into the tilt gap; Squeaks, knocking and banding
  • Elegoo Saturn 2: Vat screws seize and snap; Messy vat emptying
  • Elegoo Saturn 4: Prints fail on the same side of the plate; Vat leaks resin onto the glass
  • Elegoo Saturn 4 Ultra: LCD dies early; Force-sensor and self-test errors; Resin leaks into the chassis; Thick base and raft; No vat heater on the 12K; Vat knob strips or seizes

And 7 more; see each printer page.

Where to go from here